Meaning
Roll-bonded surface layers of aluminium-silicon brazing alloys affixed to structural aluminium core substrates provide metallurgical joining material for battery heat exchangers and cooling plate assemblies. Clad ratio specifications dictate the filler layer thickness as a nominal percentage of overall composite sheet gauge, typically varying between 5 and 15 percent per side. Common formulations employ 4000-series alloys containing 7 to 12 weight percent silicon, which lower the surface layer melting range below that of the core substrate.
The composite bond forms during hot and cold co-rolling operations at the rolling mill, ensuring continuous metallic contact across the entire coil area. The classification excludes post-applied brazing pastes, physical foil shims, galvanic coatings and thermal spray deposits.
Composite Fabrication
Multi-layer sheet production starts by securing cast alloy slabs of brazing material against prepared ingots of core metal using mechanical strapping or edge welding. Heavy hot rolling breaks down interfacial oxides under compressive shear, establishing solid-state metallic bonds across the clad-core interface. Subsequent cold rolling cycles reduce composite thickness down to final foil or sheet gauges while holding tight layer ratio tolerances.
Interstage annealing cycles soften work-hardened material without triggering interdiffusion between silicon-rich clad skins and manganese-bearing core metals. Finished clad filler coils exhibit clean interfaces free from debonding, gas blisters or thickness fluctuations.
Melt Redistribution
Thermal exposure past the clad solidus point transforms the roll-bonded skin into a mobile liquid phase across component surfaces. Silicon presence drives wetting across the core metal, drawing liquid metal toward stamped contact vertices via capillary attraction. Gravity and surface tension pull liquid filler away from flat unconstrained faces, gathering alloy mass into structural joint fillets.
Core dissolution occurs simultaneously as molten silicon leaches solid aluminium from the base sheet, altering local melt chemistry. Maintaining precise furnace temperature ramps controls this fluid migration, preventing unbonded flat surfaces from developing uneven surface morphology.
Failure Modes
Process deviations during assembly generate structural and fluid retention defects linked directly to braze layer dynamics. Excessive furnace soak durations encourage deep silicon diffusion into the core, causing core erosion and premature perforations across thin-gauge cooling channels. Underheating prevents the clad layer from fully melting, yielding incomplete fillets, cold joints and porous seam lines along fluid boundaries.
Inadequate strip preparation at the rolling mill can trap sub-surface contaminants, causing clad delamination blisters during furnace processing. Uneven rolling pressures leave localized thin patches of clad filler, resulting in starved joint interfaces that burst under operating coolant pressures.