Differential Capacity Analysis Protocols for Identifying Cold Charging Phase Transformations
Differential capacity analysis detects cold charging phase transformations and lithium plating by resolving staging shifts and discharge stripping peaks.

Bench
Differential capacity analysis below zero Celsius isolates phase behavior by transforming flat voltage plateaus into legible derivative peaks. Capturing those features requires cycling hardware with current stability held inside 0.01 percent of full scale. Channels equipped with twenty-four-bit analog-to-digital converters avoid the quantisation steps that produce phantom peaks at low temperatures, while a chamber tolerance of plus or minus 0.5 degrees Celsius prevents baseline drift across long C-rate runs.
Thermal gradients across the cell body warp local current distribution; resting the pack or cell for four hours brings it to thermal equilibrium before current starts to flow.
Low-temperature runs proceed through disciplined galvanostatic steps, starting with a 25 degrees Celsius reference cycle to baseline discharge capacity under rated conditions. Four-wire Kelvin connections go directly onto the cell tabs so lead resistance stays out of the voltage log. Because cold air stiffens wiring and contact oxidation introduces micro-ohm shifts that skew derivative calculations, pneumatic clamps are used to keep mechanical pressure steady across the terminals.
Baseline capacity grading at 25 degrees Celsius establishes the true amp-hour denominator before chilling the cell.
Data logging rates dictate derivative quality. Sampling purely on fixed time intervals yields sparse records during steep voltage changes and redundant points across broad plateaus. Setting the cycler to trigger on either a 1.0 millivolt shift or a ten seconds elapsed window ~ whichever arrives first ~ preserves peak resolution through two-phase regions without bloating files during slow sub-zero holds.
After reaching the setpoint temperature, the cell sits unpowered for sixty minutes before charging starts.
Sluggish electrolyte transport caps performance as temperatures head toward minus twenty degrees Celsius. Viscosity jumps, carbonate solvents slow bulk lithium ion migration, and concentration overpotentials climb across both electrodes. Transport resistance through the solid electrolyte interphase rises by roughly an order of magnitude.
As ohmic and charge-transfer resistances escalate, phase peaks drift up the voltage scale, making clean overpotential separation essential if one wants to distinguish thermodynamic phase boundaries from purely kinetic resistance.

Stages
Lithium intercalates into natural or synthetic graphite through distinct staging phases as packing density climbs, moving from dilute Stage 1L through Stage 4, Stage 3, Stage 2, and ending at stoichiometric Stage 1 LiC6. At 25 degrees Celsius, dQ/dV curves separate these transitions cleanly into distinct peaks. During a slow charge, the Stage 2 to Stage 1 boundary routinely lands between 0.08 and 0.12 volts against metallic lithium, standing out as a clear derivative maximum against cell potential.
Sub-zero temperatures distort this staging behavior. Even modest charging currents induce kinetic overpotentials that push graphite past zero volts versus Li/Li+. Terminal voltage bundles open-circuit equilibrium with ohmic drops, particle-surface charge transfer, and diffusion bottlenecks through the host matrix.
As the cell cools, the voltage separation between staging plateaus narrows, broadening peaks across the voltage domain and obscuring phase boundaries.

Can Plating Peaks Conceal Stage Two Staging?
Stage 2 staging occurs right along the edge of metallic lithium deposition. Once graphite polarises below zero volts versus Li/Li+, metallic lithium begins nucleating on the electrode face while intercalation is still underway, and the differential capacity curve registers both simultaneously. One stores lithium reversibly in the carbon matrix; the other deposits surface metal that consumes electrolyte.
At minus twenty degrees Celsius, solid-state diffusion inside graphite drops by two to three orders of magnitude, falling toward 10 to the power of minus fourteen square centimeters per second.
| Staging Transition | Theoretical Potential vs Li/Li+ (V) | Observed Peak at 25 C (V) | Observed Peak at -10 C at C/20 (V) | Kinetic Shift (mV) |
|---|---|---|---|---|
| Stage 4 to 3 (Dilute) | 0.210 | 0.215 | 0.345 | +130 |
| Stage 3 to 2L (Liquid-like) | 0.160 | 0.170 | 0.310 | +140 |
| Stage 2L to 2 (Ordered) | 0.115 | 0.125 | 0.285 | +160 |
| Stage 2 to 1 (LiC6 Formation) | 0.080 | 0.090 | 0.265 | +175 |
Cathode behavior further complicates full-cell dQ/dV interpretation. Nickel-rich layered oxides undergo hexagonal-to-monoclinic and hexagonal-to-hexagonal transitions between 3.65 and 4.25 volts, including a sharp H2 to H3 lattice contraction near 4.15 volts versus graphite that produces prominent derivative spikes. Under sub-zero conditions, this cathode signature flattens and drifts upward under overpotential, bleeding into adjoining solid-solution responses.
Because standard full-cell traces superimpose both electrodes into a single signal, isolating the negative electrode requires three-electrode pouch cells built with dedicated lithium reference pins.
A three-electrode test cell separates negative electrode overpotentials from cathode phase shifts under cold exposure.
Current rates drive substantial phase-boundary displacement. Shifting from C/50 to C/10 at minus ten degrees Celsius drives graphite intercalation peaks higher on the voltage scale while pulling cathode delithiation upward in tandem. This accumulated polarization cuts the duration of distinct two-phase transitions, collapsing separate stage markers into an unresolved plateau.
Resolving individual thermodynamic staging boundaries generally requires holding the charge rate below C/20.

Smoothing
Direct numerical differentiation turns minor channel noise into glaring artifacts. A voltage jitter of just fifty microvolts between adjacent records creates huge, spurious dQ/dV spikes once divided across small capacity increments, degrading smooth charging data into unreadable scatter. Digital filtering cleans up this instrumentation noise, though poorly matched filter parameters will clip real peak heights and displace phase markers along the voltage axis.
Savitzky-Golay filters address this by fitting local subsets of data to a low-degree polynomial via linear least squares. Window length governs how many points enter each regression: too narrow, and high-frequency noise remains to mimic plating shoulders; too wide, and sharp staging peaks smear out into apparent solid-solution zones. In practice, a second- or third-order polynomial paired with an adaptive window sized to 1.5 percent of the total charge array preserves underlying peak morphology.

Will Asymmetric Filtering Distort Phase Boundaries?
Non-uniform sampling complicates standard filtering routines. Voltage-delta triggers cause points to bunch up along flat plateaus and thin out during rapid transitions, which biases fixed-window filters. Fitting natural cubic splines directly to the raw voltage-capacity curve sidesteps this issue, allowing analysts to differentiate the fitted function analytically rather than relying on discrete difference steps.
Excessive digital smoothing eliminates narrow phase transformations and simulates false solid-solution behavior.
The spline smoothing factor controls the compromise between raw tracking and derivative stability. A parameter near zero forces the spline through raw noise, resurrecting the original derivative spikes, whereas excessive smoothing drags the curve toward a straight line and erases real multi-phase transitions. Cross-validation identifies an appropriate coefficient by minimizing prediction errors across omitted points, and that setting then stays fixed across all runs in a comparative set.
- Raw Differential Filtering isolates raw voltage increments to detect channel communication drops and ADC bit flips before curve reconstruction.
- Adaptive Savitzky-Golay Processing matches polynomial frame lengths to local derivative steepness, preventing edge erosion on sharp phase boundaries.
- Cubic Smoothing Splines fit regularised parametric functions to raw capacity data, yielding smooth continuous second derivatives for inflection point verification.
- Gaussian Kernel Convolution applies fixed-bandwidth spectral filters across equidistant re-sampled arrays to verify peak apex integrity across independent runs.
Automated pipelines are easily misled by filtering artifacts. Over-smoothed curves frequently form late-charge shoulders that look suspiciously like lithium stripping plateaus on reversal. To verify a filter, the analyst checks the integrated area under the dQ/dV curve against direct coulombic counting: the integrated capacity across the voltage sweep should balance the counter reading within 0.2 percent.
Any larger divergence points to boundary extrapolation errors or an over-aggressive filter.

Stripping
Lithium plating introduces a distinct metallic phase across the graphite surface whenever negative electrode potential dips below zero volts versus metallic lithium. Detecting it relies primarily on the subsequent discharge curve, where reversible metal oxidizes back into electrolyte solution slightly above the Li/Li+ equilibrium potential ~ a reaction registered as electrochemical stripping.
That stripping reaction manifests as a flat discharge plateau between 0.05 and 0.15 volts versus graphite, producing a sharp peak on the dQ/dV profile. Normal delithiation across Stage 1 to Stage 2 proceeds along a broader, smoother curve at higher overpotentials. Because this sharp low-voltage peak never appears during warm, benign cycles, its presence directly confirms that metallic lithium formed during the cold charging step.
| Diagnostic Feature | Graphite Stage 1 De-intercalation | Reversible Lithium Stripping | Irreversible Plating Residue |
|---|---|---|---|
| Peak Voltage Range (V) | 0.080 to 0.120 vs Li/Li+ | -0.020 to +0.050 vs Li/Li+ | Non-responsive electrochemically |
| dQ/dV Profile Morphology | Broad, symmetric bell curve | Narrow, sharp asymmetrical spike | Absence of discharge peak |
| Temperature Dependency | Shifts predictably with overpotential | Magnitude expands below 0 C | Scales with repeated cold exposure |
| Relaxation Impact | Stable over multi-hour rest | Peak area shrinks with longer rest | Permanent capacity loss logged |
Rest periods inserted between charge completion and discharge clarify how stable that plated metal actually is. Metallic lithium sitting in organic electrolyte is thermodynamically unstable and corrodes spontaneously, reacting with solvent molecules to build secondary solid electrolyte interphase layers. This parasitic chemical stripping consumes inventory without passing electrons through the external circuit, which is why extending rest duration progressively reduces the stripping peak area on the dQ/dV curve.
Quantifying that reversible fraction requires integrating under the stripping peak between the inflection minima on either side of the dQ/dV maximum. Integrating differential capacity across that window gives the recovered capacity in milliampere-hours, and dividing it by the prior charge capacity yields the reversible plating ratio. Any lithium isolated as electronically dead metal or lost to SEI growth turns up as permanent capacity loss during subsequent reference cycles.
Electrode architecture heavily dictates plating sensitivity. Highly calendered, low-porosity coatings choke through-plane ion transport, forcing the negative potential below zero at the current collector foil long before the separator face saturates. Tortuous pores foster localized plating pockets while outer particles remain under-utilized.
In pouch formats, thin foils worsen planar temperature spreads and uneven mechanical compression generates early localized stripping peaks well before full state of charge.

Metric
Defining a defensible cold-charging envelope requires clear criteria pulled from dQ/dV data rather than qualitative inspection of curve shapes, which only leads to disputes between cell vendors and pack integrators. Translating derivative curves into explicit mathematical pass/fail boundaries makes it possible to determine whether a given charge rate at sub-zero temperatures triggers plating, anchoring acceptance directly to numerical qualification records.
Tracking the ratio between the Stage 2 to Stage 1 lithiation peak and the earlier dilute staging peak provides an early warning for kinetic breakdown. At room temperature, this ratio remains stable across cycling. Under sub-zero currents, it drops sharply as mass-transport bottlenecks restrict graphite saturation.
Once the Stage 1 peak area contracts to under fifteen percent of its baseline value at a matching state of charge, the electrode cannot accept incoming flux without driving lithium deposition.
A second metric tracks the onset voltage against cell state of charge. During a minus ten degrees Celsius charge, the second derivative of voltage marks the precise point where normal staging breaks down. Plating begins mathematically where dQ/dV departs upward from the baseline intercalation envelope; cyclers running real-time derivative monitors can flag that inflection and cut or taper current immediately.
- Baseline Mapping Execution establishes the reference dQ/dV envelope across five cells cycled at C/50 at 25 degrees Celsius inside a controlled environmental chamber.
- Sub-zero Isothermal Soaking equilibrates test specimens at target operating temperatures between 0 and minus 20 degrees Celsius for four hours without applied load.
- Stepwise Galvanostatic Cycling charges cells under incremented C-rates from C/20 to C/2 up to the specified upper cut-off voltage limit.
- Derivative Peak Deconvolution calculates cubic-spline filtered dQ/dV discharge profiles to detect stripping peak areas above 0.5 percent of nominal capacity.
- Envelope Boundary Allocation fixes the maximum continuous charge current at the highest rate demonstrating zero reversible stripping peaks and full phase boundary retention.
Batch qualification requires firm tolerances on sub-zero charging. Receiving inspections pull three cells per ten thousand units for destructive sub-zero characterisation: if any unit shows a stripping peak area exceeding 1.0 percent of discharge capacity during a C/10 charge at minus ten degrees Celsius, the lot is rejected under safety clauses. Stripping peaks are often rationalized as benign stage-two overpotential shifts, which makes explicit mathematical definitions of peak integration boundaries essential for contractual enforcement.
Formulation decisions dictate cold dQ/dV performance long after production. Blending fluorinated ethylene carbonate or low-viscosity carboxylate co-solvents depresses the electrolyte freezing point, extending legible graphite staging down to minus twenty degrees Celsius, while amorphous carbon coatings on synthetic graphite curb charge-transfer resistance and push plating onset to higher rates. Omitting cold dQ/dV requirements from procurement contracts routinely results in standard-impedance cells that fade rapidly under winter fast-charging.
Omitting differential capacity criteria simply pushes warranty exposure downstream to the pack integrator. Cells charged blindly in cold conditions accumulate inactive metallic lithium, accelerating cathode transition-metal dissolution and puncturing separators months down the line. Factoring premature pack replacements into landed cost shifts the balance on supplier quotes, tying eventual field reliability directly back to clauses set during initial cell qualification.