Planar Strain Ratio Testing for Sheet Steel Forming
Planar strain ratio testing quantifies directional flow differences across sheet steel coils to eliminate flange earing and prevent press tooling failures.

Anisotropy
Deep drawing sheet steel requires tight control over directional plastic flow in the press. Preferred crystallographic orientations that develop during hot rolling, cold reduction, and continuous annealing force the sheet to deform unevenly under multi-axial stress. In drawn cylindrical cans, battery enclosures, and structural module trays, this directionality dictates whether the blank feeds smoothly into the die cavity or splits over the punch radius.
Standard uniaxial tensile testing captures this behavior through the Lankford plastic strain ratio ~ the ratio of true width strain to true thickness strain. Measuring this value along three planar orientations reveals both overall drawability and the material’s tendency toward uneven flow.
The normal plastic strain ratio reflects how well a sheet resists thinning under tensile loads. Higher values show that metal resists thinning through its thickness while expanding readily within the sheet plane. Variation in this strain ratio across the plane ~ known as planar anisotropy ~ governs the height and placement of ears along the drawn shell rim.
When planar variation strays from zero, material flows faster along specific crystallographic directions, producing uneven peaks and valleys that can disrupt transfer automation.
A planar anisotropy value of positive 0.45 produces four distinct ears aligned with the rolling and transverse directions during cylindrical cup drawing.
Determining these directional parameters follows ASTM E517 and ISO 10113 standards. Tensile specimens are cut along three axes relative to the coil rolling direction: longitudinal at zero degrees, diagonal at forty-five degrees, and transverse at ninety degrees. True axial strain and true width strain are logged simultaneously during uniform plastic deformation, staying clear of the necking zone to accurately capture through-thickness wall behavior.
Standard formulas combine these directional measurements into summary indices used in finite element stamping simulations and coil procurement specs:
- Normal Plastic Strain Ratio defines the average resistance of the sheet to through-thickness thinning across all planar directions, calculated by weighting the diagonal orientation double relative to the longitudinal and transverse axes.
- Planar Plastic Strain Ratio captures the directional spread of plastic flow within the sheet plane, calculated as half the sum of longitudinal and transverse ratios minus twice the diagonal ratio.
- True Plastic Width Strain represents the logarithmic ratio of instantaneous specimen width to initial gauge width measured under steady plastic deformation.
- True Plastic Thickness Strain represents the logarithmic through-thickness dimensional change derived from the constancy of volume principle under plastic deformation.
Successful deep drawing depends heavily on maintaining high normal strain resistance across the sheet.
Steels with uniform directional flow minimize wall thinning, eliminating the need for secondary trimming operations over the life of the tooling.

Blank
Specimen preparation and blanking methods directly affect scatter in anisotropic tensile data. Conventional shear cutting leaves a heavily work-hardened zone extending up to one-half the sheet thickness into the gauge area, alongside micro-cracks and heavy edge burrs. These edge flaws trigger premature local yielding and disrupt transverse extensometer tracking during uniform elongation.
In contrast, precision waterjet cutting or low-stress wire EDM preserves the base metal microstructure and keeps cross-sectional geometry uniform along the gauge length to avoid edge tearing.
Specimen dimensions follow tight tolerances set by ASTM E8 and ISO 6892-1 to prevent stress concentrations near the grips. The parallel section requires smooth transition fillets with radii over twenty-five millimeters to prevent triaxial constraint at the shoulder. Standard geometries feature either a twelve-and-a-half millimeter width over a fifty-millimeter gauge length or a twenty-millimeter width over an eighty-millimeter gauge length, avoiding edge burrs that can start early fractures.
| Steel Grade | Yield Strength (MPa) | Longitudinal Ratio (r0) | Diagonal Ratio (r45) | Transverse Ratio (r90) | Average Ratio (r-bar) | Planar Variation (Delta-r) |
|---|---|---|---|---|---|---|
| Interstitial Free (DC06) | 145 ± 10 | 2.10 ± 0.05 | 1.62 ± 0.04 | 2.45 ± 0.06 | 1.95 ± 0.04 | +0.66 ± 0.05 |
| Drawing Quality (DC04) | 185 ± 15 | 1.75 ± 0.04 | 1.25 ± 0.03 | 2.05 ± 0.05 | 1.58 ± 0.03 | +0.65 ± 0.04 |
| Bake Hardenable (B180) | 210 ± 12 | 1.55 ± 0.04 | 1.18 ± 0.03 | 1.82 ± 0.04 | 1.43 ± 0.03 | +0.51 ± 0.04 |
| Dual Phase (DP600) | 380 ± 20 | 1.02 ± 0.03 | 0.85 ± 0.03 | 1.15 ± 0.03 | 0.97 ± 0.02 | +0.24 ± 0.03 |
| Transformation Induced (TRIP780) | 460 ± 25 | 0.92 ± 0.03 | 0.78 ± 0.03 | 1.04 ± 0.04 | 0.88 ± 0.02 | +0.20 ± 0.03 |
Sampling from primary coils must account for cross-thickness crown profiles and thermal gradients generated during batch annealing. Outer coil wraps and edge strips cool at different rates than the core, altering crystallographic texture across the width. Comprehensive receiving inspection requires sampling blanks from centerline, quarter-width, and drive-side slit positions to map property variation before releasing coils to production dies.
Mill certificates omitting test orientation angles hide planar variation by reporting only transverse tensile values.
Punch stroke dynamics control how the blank moves into the die cavity.
While slit edge burrs fell within broad commercial warehouse standards, tool wear on the stamping line ultimately caused the sidewall tears.

Extensometry
Accurate measurement of uniform plastic strain requires precise dual-axis sensors. Manual micrometer readings taken before and after testing introduce operator bias and miss the actual strain path. Modern frames combine class 0.5 axial extensometers with transverse optical or multi-point contact averaging units.
The transverse sensor tracks width contraction across three points in the gauge section to compensate for slight localized necking or specimen curvature, while optical tracking avoids contact slippage entirely.
Measuring thickness directly during tensile testing is unworkable on sheet thinner than one millimeter because contact points indent the metal and knife edges slip. Standards overcome this by calculating thickness strain from volume constancy, assuming plastic incompressibility where longitudinal, width, and thickness true strains sum to zero. This calculation fails if void formation accelerates, which happens in high-inclusion commercial steels or multiphase grades loaded near their ultimate tensile strength.
- Mount the specimen in hydraulic wedge grips using alignment fixtures to keep angular deviation below one-half degree.
- Attach dual-axis extensometers along the central gauge section, checking the load cell to ensure zero point-load bending.
- Run the crosshead at a constant strain rate between 0.0002 and 0.008 per second while continuously logging load, elongation, and width contraction.
- Stop recording at fifteen percent engineering strain or just before maximum uniform load to exclude localized necking.
- Calculate logarithmic plastic strains by subtracting elastic compliance using calibrated dynamic elastic modulus values.
Localized shear bands frequently cause premature splitting during uniform extension.
Specimen gauge thickness below 0.60 millimeters amplifies cross-sectional micrometer measurement errors by a factor of three in the calculated thickness strain.
Digital image correlation provides full-field displacement maps by tracking thousands of point coordinates across the specimen surface. This non-contact optical approach isolates local strain gradients and catches minor machine misalignment before bad displacement data skews the results. Misalignment creates asymmetric strain across the width, inflating calculated r-values by several tenths of an index point.
Inaccurate gauge readings distort the calculated anisotropy index, leading to unexpected splitting on production presses and high scrap rates that undermine job profitability.

Flange
As sheet metal flows over the draw ring, directional property variations transform into physical defects in the drawn shell. When the blankholder clamps the sheet edge, radial drawing pulls material inward toward the die radius, setting up compressive hoop stresses around the perimeter. The planar strain ratio determines whether this stress causes circumferential thickening or lateral stretching.
Large directional differences lead to uneven flange retraction, producing raised ears separated by low troughs whose heights scale directly with anisotropy.

Will Severe Earing Jam High-Speed Transfer Presses?
Severe rim earing causes major disruptions in progressive dies and transfer lines. Deep ears prevent transfer rails from gripping shells evenly, destabilizing part alignment in downstream redraw or pierce stations. If ear heights exceed trim allowances, the ragged rim folds into the punch radius, creating loose metal slivers that gall tool surfaces and mark subsequent parts.
Ear locations depend directly on the sign of the planar strain index:
| Planar Index (Delta-r) | Ear Peak Locations Relative To Rolling Direction | Dominant Flange Stress Mode | Primary Tooling Risk |
|---|---|---|---|
| Positive (> +0.20) | 0 degrees and 90 degrees | Excessive circumferential hoop thickening | Transfer nest jamming, punch radius galling |
| Near Zero (-0.10 to +0.10) | Uniform cylindrical flange profile | Balanced through-thickness hoop compression | Minimal tooling wear, predictable trim line |
| Negative (< -0.20) | 45 degrees and 135 degrees | Diagonal localized metal drawing flow | Sidewall thinning, corner split during ironing |
Excessive flange deformation rapidly increases scrap generation during edge trimming.
In rectangular draws like battery module cases and prismatic cell housings, flow anomalies trigger corner puckering and sidewall oil-canning. Materials with low normal strain ratios thin rapidly around tight corners, forming narrow necked regions that leak during post-weld helium testing. Higher normal values spread deformation into the adjacent straight sidewalls, keeping corner thickness intact and preserving crush strength, direct benefits of crystallographic alignment achieved during rolling.
Die clearance designed for isotropic material experiences localized iron pinch forces when positive planar values drive ninety-degree flange thickening.
The maximum limiting draw ratio constrains shell depth prior to necking.
Whether high-speed press friction shifts ear locations away from positions predicted by quasi-static lab tests remains a point of debate among stamping metallurgists.

Tolerance
Procurement contracts for precision forming steels tie material properties directly to lot acceptance criteria. Generic grade designations like commercial steel or drawing steel offer little protection against lot-to-lot forming variation. Precise stamping operations specify statistical limits for both normal and planar indices in purchase agreements.
Mill suppliers must control annealing temperatures, cold reduction ratios, and residual interstitials like carbon and nitrogen to hold properties consistent across shipments, avoiding line downtime caused by unverified material.
Consider a high-speed battery enclosure line running 0.80 millimeter cold-rolled sheet. Tool clearances are set to 0.88 millimeters, leaving a ten percent gap. Stamping simulations assume a baseline average plastic strain ratio of 1.80 and a planar variation of positive 0.15.
A delivered master coil tests at an average ratio of 1.35 with a planar variation of positive 0.75 ~ acceptable under standard commercial specs, but well outside the process window. Processing this out-of-spec lot causes immediate tooling problems:
- Flange Ear Height increases from two millimeters to seven millimeters, exceeding the automated trim envelope and dropping metal slivers into the lower die.
- Thickness Ironing Force surges thirty-five percent along ninety-degree draw walls as thickened ears pinch through the 0.88 millimeter clearance gap.
- Corner Thinning Strain escalates from twenty-two percent to thirty-eight percent, causing micro-cracks around bottom punch radii.
- Die Maintenance Cadence drops from two hundred thousand strokes down to twenty-five thousand strokes due to heavy galling on coated inserts.
Progressive tooling wear continually shifts boundary friction conditions during long production runs.
Unpredicted shifts in yield locus distort finite element press predictions.
Receiving inspection protocols require testing three blanks per twenty-ton master coil, cutting tensile samples at zero, forty-five, and ninety degrees. Automated optical tests calculate r-values and compare them against statistical control limits. The plant rejects any coil whose average ratio falls below 1.60 or whose absolute planar variation exceeds 0.30, quarantining the steel before blanking.
Citing ASTM E517 Section 8 and ISO 10113 annex provisions gives plants legal retest rights, allowing out-of-spec coils to be rejected back to the mill before entering production.