Quantifying Local Overpotentials and Lithium Plating under Pack Cold Plate Gradients
Bottom cold plates create local thermal gradients that drop anode overpotentials below zero volts, causing localized lithium plating during un-derated fast charge.

Sink
Liquid cold plates positioned beneath large-format battery cells introduce steep thermal gradients along both longitudinal and cross-plane dimensions. In an electric vehicle pack where a single aluminum cooling plate chills the cell base, the top of a 300-millimeter-tall prismatic cell operates at a significantly higher temperature than the cooled base. Thermal gradients drive current redistribution.
Cross-plane thermal conductivity within pouch and prismatic cells is governed by alternating layers of active material, current collector foils, micro-porous separators, and liquid electrolyte. While copper and aluminum foil layers conduct heat effectively along the planar direction at conductivities ranging from 200 W/mK to 380 W/mK, the composite stack exhibits cross-plane thermal conductivity between 0.5 W/mK and 1.2 W/mK. Layer thickness governs heat transfer.
Consequently, heat generated in the core of a thick cell faces high thermal impedance when traveling toward an external cold plate surface.

Thermal Anisotropy across Large-Format Architectures
Geometric dimensions directly dictate internal thermal divergence during high-rate charging events. In large pouch cells, planar dimensions exceeding 500 millimeters exacerbate local temperature variations across the active electrode surface. Coolant flowing through internal cold plate channels absorbs energy as it travels from the inlet manifold to the outlet manifold.
This thermal absorption establishes a secondary thermal gradient across the pack footprint, resulting in cells located near the coolant outlet operating up to 8 K warmer than cells adjacent to the coolant inlet. Local electrochemical reaction rates scale exponentially with local temperature according to Arrhenius kinetics. Warmer regions of an electrode stack display reduced charge-transfer resistance and higher ionic conductivity within the liquid electrolyte, causing electric current to preferentially concentrate in high-temperature zones during the initial phases of constant-current charging.

Interfacial Thermal Impedance Stack-Ups
Heat transfer between the cell casing and the liquid cooling structure is controlled by the physical interface stack-up. Mechanical contact between aluminum cell enclosures and cold plate surfaces depends entirely on thermal interface materials to bridge microscopic surface roughness and mechanical tolerances. Creep alters contact pressure.
Variations in thermal interface material thickness alter local thermal resistance across the cell footprint.
- Compressive Load Relaxation Thermal interface materials experience viscoelastic creep under sustained stack pressure, altering local thermal resistance by up to 35 percent across extended operating lifecycles.
- Coolant Temperature Rise Liquid flow along internal cold plate channels picks up heat, creating a 3 K to 8 K temperature differential between inlet and outlet manifolds under peak thermal loads.
- Separator Thickness Variations Tolerances in polyolefin separator manufacturing induce minor local variations in ionic path length and cross-plane thermal conduction.
- Tab Proximity Heating Localized current density near copper and aluminum tab welds creates concentrated Joule heating that contrasts sharply with base-cooled cell foundations.
Bottom cooling of large prismatic cells forces heat transport across hundreds of electrode layers possessing low cross-plane thermal conductivity.
Designing thermal management systems around average surface temperatures guarantees localized electrochemical acceleration of lithium deposition near liquid coolant channels.

Anode
Solid-state thermodynamic stability during charge depends directly on the phase boundary potential between graphite particles and liquid electrolyte. The thermodynamic requirement for intercalation requires the local equilibrium potential of the negative electrode to remain strictly positive relative to the metallic lithium redox couple. When the local negative electrode overpotential drops below zero volts versus lithium reference, the reduction of lithium ions to metallic lithium becomes thermodynamically favorable.
Cold graphite intersperses ions slowly. Metallic lithium plating competes directly with graphite intercalation kinetics. Plating occurs predominantly at the interface between the negative electrode and the separator, where liquid-phase electrolyte potential experiences its maximum drop during high-rate charging operations.

Butler-Volmer Kinetic Suppression at Suppressed Temperatures
Charge transfer kinetics at the graphite particle surface follow Butler-Volmer formulations, where the exchange current density scales strongly with local temperature. A decrease in local temperature from 298.15 K to 278.15 K reduces exchange current density by more than half, forcing higher charge-transfer overpotentials to sustain a given current density. Interfacial resistance increases at low temperatures.
The cathodic charge transfer overpotential increases proportionally, driving the solid-phase potential downward relative to the adjacent liquid electrolyte phase. At subzero temperatures, the kinetic barrier for intercalation rises significantly above the nucleation barrier for metallic lithium deposition, rendering lithium plating the kinetically favored pathway during un-derated fast charging.

Electrolyte Phase Potential Drops across Porous Structures
Ionic transport through liquid electrolyte contained within porous electrode networks is bounded by bulk ionic conductivity and tortuosity factors. Low temperatures increase solvent viscosity and reduce salt dissociation, causing bulk ionic conductivity to drop rapidly. The effective liquid-phase conductivity inside the porous anode structure decreases in accordance with Bruggeman tortuosity relationships.
During charge, negative ions migrate away from the negative electrode surface while positive lithium ions are consumed within the porous graphite matrix. This transport limitation establishes an electrolyte phase potential gradient across the electrode thickness. A severe drop in liquid-phase potential near the separator face depresses the localized electrode equilibrium potential, pushing the local reaction overpotential into negative territory even when the bulk cell terminal voltage remains below the nominal upper cut-off limit.
| Temperature (K) | Ionic Conductivity (mS/cm) | Electrolyte Diffusivity (10⁻⁶ cm²/s) | Exchange Current Density (A/m²) | Anode Overpotential Shift at 1C (mV) |
|---|---|---|---|---|
| 298.15 | 10.5 | 3.2 | 1.85 | +45 |
| 288.15 | 7.8 | 2.1 | 1.10 | +18 |
| 278.15 | 4.4 | 1.2 | 0.52 | -12 |
| 268.15 | 2.1 | 0.5 | 0.19 | -68 |
At operating temperatures below 278.15 K, electrolyte ionic conductivity drops below 4.5 mS/cm, increasing liquid-phase potential drop across a 70-micrometer porous electrode to over 80 mV.
Ignoring spatial overpotential variation during cold charging leads to internal short circuits, sudden capacity fade, and catastrophic thermal runaway when plated lithium dendrites penetrate the microporous polyolefin separator.

Voltage
Terminal potential measurements mask localized internal polarization phenomena across large electrode surface areas. A battery management system monitoring overall cell voltage reads an area-averaged sum of positive electrode potential, negative electrode potential, and internal ohmic drops. Local voltage drops below zero.
In a cell experiencing single-sided liquid cooling, cold regions near the bottom plate operate at high local overpotentials while warmer regions near the cell tabs operate at low local overpotentials. The composite terminal voltage appears safe because warm active material zones absorb current while maintaining positive local anode potentials. Meanwhile, cold regions adjacent to the cold plate cross the zero-volt threshold, initiating metallic lithium deposition without triggering pack-level voltage alarms.

Why Does Thermal Asymmetry Shift Negative Electrode Overpotential?
Local polarization redistribution drives spatial non-uniformity across the negative electrode planar area. When a thermal gradient exists across a cell, internal resistance variations cause current density to concentrate heavily in low-resistance warm regions during early charge stages. As warm regions charge faster, their local state of charge rises, increasing their local open-circuit potential.
This open-circuit potential rise gradually forces electric current back into the higher-resistance cold regions later in the charging cycle. When high current density is artificially forced into low-temperature graphite zones late in the charge cycle ~ where state-of-charge is already high and lithium diffusivity is severely suppressed ~ the local negative electrode potential drops below zero volts versus lithium. Lithium metal nucleates on graphite.

Operando Reference Electrode Diagnostics
Quantifying local overpotential distributions requires physical or optical diagnostic probes embedded directly within prototype cell assemblies. Standard three-electrode setups utilize metallic lithium or gold micro-wires placed at specified spatial locations between the separator and the graphite electrode surface. Reference electrodes reveal local polarization.
By measuring the potential difference between the local graphite matrix and the isolated reference wire, engineers isolate the true single-electrode potential evolution during real-time charging routines. Testing proves that three-electrode insertion must maintain precise spatial placement, as a offset of fifty micrometers alters measured electrolyte potential by tens of millivolts due to local potential field gradients.

Stripping Relaxation and Differential Capacity Analysis
Non-destructive detection of metallic plating relies on post-charge voltage relaxation kinetics and differential capacity calculation. Immediately following the cessation of high-rate charging, a cell containing plated metallic lithium exhibits a characteristic voltage plateau during open-circuit relaxation. This plateau represents the chemical re-intercalation or corrosion stripping of metallic lithium into the graphite structure.
Differential capacity curves track metallic stripping. Calculating the differential capacity (dQ/dV) during low-rate discharge reveals a distinct oxidation peak corresponding to metallic lithium dissolution, positioned at a lower potential than standard graphite de-intercalation peaks.
- Three-Electrode Insertion Place gold-coated micro-wires or metallic lithium reference wires directly into the cell stack to isolate single-electrode potential evolution during dynamic fast charge.
- Post-Charge Voltage Relaxation Monitor open-circuit terminal voltage recovery immediately after current interruption to detect the characteristic voltage plateau associated with reversible lithium stripping.
- Differential Capacity Deconvolution Calculate the derivative of capacity with respect to voltage during low-rate discharge to resolve distinct phase transition peaks associated with metallic lithium re-intercalation.
- High-Precision Coulometry Measure charge return efficiency across back-to-back cycling regimes at subzero temperatures to quantify net active lithium inventory losses.
Standard IEC 62660-1 qualification testing under ambient room conditions fails to capture localized negative electrode polarization induced by single-sided liquid cold plate cooling.
It remains uncertain how non-uniform mechanical pressure relaxation across swelling pouch stacks interacts with local electrolyte depletion to accelerate localized lithium plating under long-term field operation.

Kinetics
Coupled three-dimensional multi-physics models link heat generation equations with spatial electrochemical transport equations to evaluate localized degradation rates. Continuum modeling relies on Pseudo-2D Doyle-Fuller-Newman formulations solved concurrently across a discretized spatial mesh representing the mechanical geometry of the pack module. Solid-state diffusion within spherical active particles is modeled alongside liquid-phase diffusion through tortuous pore networks.
The coupling between thermal balance equations and electrochemical kinetic equations accounts for temperature-dependent physical parameters via Arrhenius relationships. Local current density redistributes dynamically across the spatial domain based on local total impedance calculations executed at every time step of the charging simulation.

Spatial Current Redistribution along Thermal Gradients
Current distribution dynamics evolve through distinct stages during a constant-current constant-voltage charging event under cold plate gradients. In the initial constant-current phase, cold zones present high charge-transfer resistance, diverting up to 70 percent of the total pack current through the warmer regions of the cell stack. As warm regions approach their upper state-of-charge limits, their local open-circuit potential increases, shifting the potential driving force back toward the cold zones.
Cold spots limit charging rate. Consequently, late in the constant-current phase, cold regions experience a localized surge in current density precisely when their internal transport properties are least equipped to process incoming lithium ions, creating peak lithium plating risk right before the transition to constant-voltage mode.

Separator Compression and Tortuosity Escalation
Mechanical boundary conditions interact strongly with local reaction kinetics inside compressed pack enclosures. External clamping forces applied to maintain module structural integrity transmit compressive stress through the cell stack layers. Mechanical clamping changes contact resistance.
Polyolefin separators undergo non-uniform plastic and elastic deformation under localized high-pressure points, reducing internal porosity and elevating effective tortuosity. High tortuosity restricts liquid-phase ionic conduction, amplifying electrolyte overpotential drops. Combined cold plate cooling and localized mechanical over-compression generate localized negative electrode overpotentials exceeding negative 100 millivolts under 1.5C fast charging conditions.
- Measure temperature-dependent ionic conductivity and diffusion coefficients of bulk electrolyte across target operating thermal windows from 253.15 K to 318.15 K.
- Calibrate single-particle exchange current densities and activation energies for both positive and negative electrode active materials using symmetric cell electrochemical impedance spectroscopy.
- Construct a three-dimensional finite-element geometry representing cell casing, current collector foils, coating layers, separator sheets, and thermal interface materials.
- Solve coupled energy balance and Pseudo-2D electrochemical equations simultaneously to evaluate local solid-phase and liquid-phase potentials across the entire cell volume.
- Extract local negative electrode equilibrium overpotentials along the thermal gradient to identify spatial zones where potential falls below zero volts versus lithium reference.
| Cell Architecture | Cross-Plane Conductivity (W/mK) | In-Plane Conductivity (W/mK) | Max Planar Temperature Delta (K) | Minimum Local Anode Potential (mV vs Li/Li⁺) |
|---|---|---|---|---|
| Large Pouch (60 Ah) | 0.6 | 285.0 | 9.4 | -42 |
| Large Prismatic (120 Ah) | 0.95 | 140.0 | 12.1 | -78 |
| Cylindrical 4680 (Tabless) | 2.1 | 62.0 | 4.2 | +14 |
| Data compiled from 3D coupled thermal-electrochemical simulations under standard 50 kPa external stack pressure. | ||||
Cell manufacturers often assert that macro-scale terminal voltage limits provide sufficient operating margin against lithium deposition under cold plate thermal gradients.

Margin
Safe fast-charging execution demands dynamic derating protocols derived from worst-case local overpotential estimates rather than pack-level temperature averages. Traditional battery management systems adjust maximum allowable charging current using a single-dimensional lookup table keyed to the average or maximum temperature reported by a limited number of module thermistors. Fast charging requires active thermal management.
This traditional approach exposes cold zones to excessive charging currents. Anode potential determines plating risk. Implementing multi-point thermal sensing combined with real-time electrochemical observers allows the control software to project the minimum local anode potential across the entire spatial geometry of every cell in the pack.

Multi-Point Temperature Vector Derating Algorithms
Advanced pack control architectures substitute traditional scalar temperature inputs with spatial thermal vector inputs. Thermistors placed at both the cold plate interface and the warmer tab regions feed temperature maps into a real-time equivalent-circuit model running inside the battery management system. The algorithm estimates local solid-phase and liquid-phase polarization drops across spatial nodes.
When the model predicts that the local anode potential at the coldest node is approaching five millivolts positive relative to metallic lithium, the maximum allowable charge current is stepped down immediately, irrespective of the average cell surface temperature.

Active Thermal Conditioning Interventions
Preventing localized plating under aggressive cold plate cooling regimes requires active thermal intervention prior to and during high-rate fast charging. Pre-conditioning circuits run heat pumps or positive-temperature-coefficient heaters to elevate minimum cell temperatures above 288.15 K before opening high-current charging contactors. Thermal interface pads drift over time.
If charging begins while a large internal temperature gradient exists, cold plate coolant flow rates can be temporarily throttled back to permit internal Joule heating to equalize the cell thermal profile, eliminating low-temperature zones that cause local overpotential collapse.
- Minimum Local Temperature Index Set maximum charging current based exclusively on the coldest estimated sensor location within the cell module geometry.
- State-of-Charge Thresholding Step down charging current exponentially as negative electrode open-circuit potential approaches zero volts versus lithium.
- Pre-Conditioning Thermal Targets Mandate active coolant heating until the maximum internal cell temperature delta falls below 3 K prior to initiating high-rate charging.
- Pulse Relaxation Intervals Insert periodic short open-circuit rest periods into fast-charge profiles to allow local electrolyte concentration gradients to dissipate.
| Control Strategy | Sensory Input Baseline | Charging Time (10% to 80% SoC) | Local Plating Occurrence | Capacity Retention after 1000 Cycles |
|---|---|---|---|---|
| Scalar Average Temperature | Single surface thermistor | 28 minutes | Severe (base region) | 68 % |
| Scalar Minimum Temperature | Cold plate thermistor | 44 minutes | None (over-conservative) | 91 % |
| Model-Based Local Overpotential | Multi-point vector + observer | 32 minutes | None (optimized margin) | 89 % |
Derating charging currents based on average cell surface temperatures permits localized lithium plating at cold cell bases where electrolyte transport is severely retarding ion mobility.
Master cell supply contracts incorporating section 4.2 of standard ISO 12405-4 shift financial liability for cold-temperature lithium plating degradation directly to integrators who operate fast-charge protocols without real-time local overpotential observer software.

Envelope
Commercial contracts governing cell procurement must clearly delineate testing obligations and warranty liability related to thermal gradient degradation. When a cell purchaser embeds third-party cells into a custom pack module equipped with single-sided liquid cooling, the mechanical and thermal boundary conditions diverge radically from the cell manufacturer’s isolated datasheet test environment. Standard datasheets specify cycle life and fast-charge windows based on isothermal ambient chamber testing, where cells sit in still air or uniform liquid baths.
Operating those same cells under steep cold plate gradients voids standard performance warranties unless specific cold-gradient testing addendums are negotiated during RFQ drafting.

Warranty Seams and Compliance Boundaries
Establishing clear legal boundaries between cell suppliers and pack integrators requires defining precise electrochemical envelope limits within master service agreements. The warranty seam hinges on whether capacity fade stems from inherent cell manufacturing defects or integrator-induced thermal abuse. If an integrator applies a 2C fast-charge profile while maintaining a cold plate inlet temperature of 273.15 K, localized plating will degrade cell capacity rapidly.
Unless the cell supplier explicitly certified the cell format for single-sided cold plate fast charging down to that inlet temperature, responsibility for resulting pack failures falls entirely on the pack integrator.

Production Validation Protocols for Cold Plate Integration
Validating cell durability inside custom pack architectures demands first-article qualification routines that replicate operational thermal gradients. Testing protocols require prototype modules to undergo combined thermal-electrochemical cycle testing inside climate chambers while liquid cold plates operate at minimum rated coolant temperatures. Post-test tear-down inspection utilizes optical fluorescence microscopy, scanning electron microscopy, and inductively coupled plasma mass spectrometry to detect physical metallic lithium deposits on harvested anode sheets.
Quantifying localized lithium plating before signing volume production agreements protects tooling investments and prevents field recall expenses.
When pack integrators conduct independent three-electrode qualification trials under representative cold plate cooling conditions, the resulting overpotential maps establish unassailable technical evidence for setting production fast-charge boundaries.